Concrete Slump Test: Procedure, Values and Types of Slump

The slump test measures how workable fresh concrete is. A cone of concrete is filled, compacted and lifted off, and the distance the concrete sinks is the slump, in millimetres. A higher slump means a wetter, more flowing mix; a lower slump means a stiffer one. It takes about five minutes on site and is the first check made on every truck or batch.

The test is covered by IS 1199 in India and by ASTM C143 in the United States (EN 12350-2 in Europe). The steps below follow the common method; where the codes differ, the difference is noted, and the version named in your project specification always applies.

What the slump test tells you (and what it does not)

Slump is a quick measure of consistency. It helps you spot a batch that has too much or too little water compared with the approved mix, and it shows whether the concrete suits the way it will be placed. It does not measure strength. Two mixes can have the same slump and very different strength, so slump never replaces the cube test; see our guide to the concrete cube test for that.

Civil Site Engineer Bundle — Concrete QC Handbook + RCC Lap Length Excel cover
📚 Recommended Download
Civil Site Engineer Bundle — Concrete QC Handbook + RCC Lap Length Excel
Our two best-sellers in one download: the 238-page Concrete Site Handbook kit plus the IS 456 lap-length Excel toolkit and quick-reference PDF.
✔ IS 456 based  ·  ✔ Instant download  ·  ✔ Lifetime access
₹1098₹299
Get the Bundle →
1

Apparatus

  • Slump cone (frustum mould): 300 mm high, 200 mm diameter at the base, 100 mm diameter at the top, open at both ends
  • Tamping rod: 16 mm diameter, about 600 mm long, with a rounded (bullet) end
  • Flat, rigid, non-absorbent base plate or tray
  • Scoop, steel ruler or tape, and a trowel or straight edge
  • Damp cloth to wipe the inside of the cone

Step-by-step procedure

  1. Clean the cone and the base plate, and dampen the inside of the cone. Place the cone on the level, firm base, and hold it down by standing on the foot pieces.
  2. Fill the cone in layers. In ASTM C143 there are three layers of about equal volume; the older IS 1199 method uses four layers, each about one-quarter of the cone height.
  3. Compact each layer with 25 strokes of the rod, spread evenly over the surface. For the second and later layers, push the rod just through into the layer below.
  4. After the top layer, strike off the surface level with the rod or trowel, and clean any concrete from the base around the cone.
  5. Lift the cone straight up, slowly and steadily, in about 5 seconds (ASTM allows 5 plus or minus 2 seconds), without twisting or sideways movement.
  6. At once, place the empty cone upside down next to the concrete and lay the rod across it. Measure from the underside of the rod to the displaced centre of the top of the concrete.
  7. Record that distance to the nearest 5 mm as the slump. The whole operation, from starting to fill to lifting the cone, should be done without delay (ASTM asks for no more than 2.5 minutes in total, and the test to begin within 5 minutes of taking the sample).

Worked example: the top of the cone is 300 mm above the base. After lifting, the highest point of the concrete is measured as 225 mm above the base, so the slump is 300 − 225 = 75 mm.

Types of slump

  • True slump: the concrete settles evenly and keeps its shape. Record the value.
  • Shear slump: one half slides sideways off the other. The result is not valid. Repeat the test with a fresh sample. If shear happens again, the mix lacks cohesion and should be checked.
  • Collapse: the concrete spreads out flat. The mix is too wet for the slump test; a flow test is more suitable.

Recommended slump for different work

IS 456 (Table 7) gives workability ranges by type of work. Typical values are shown below; your approved mix design and the engineer’s instructions decide the actual limits.

Type of workTypical slump (mm)
Blinding concrete, shallow sections, pavements laid by paver25 to 75
Mass concrete, lightly reinforced slabs, beams, walls, columns, strip footings50 to 100
Heavily reinforced slabs, beams, walls and columns100 to 150
Slip-form work and pumped concrete75 to 150
Trench fill100 to 150
Piling and tremie concrete150 to 200

European specifications group slump into classes: S1 is 10 to 40 mm, S2 is 50 to 90 mm, S3 is 100 to 150 mm, S4 is 160 to 210 mm and S5 is 220 mm or more.

What changes the slump

  • Water content: more water gives more slump. This is the main factor, and also why extra water weakens concrete. See the water-cement ratio guide.
  • Admixtures: plasticisers and superplasticisers raise slump without more water.
  • Aggregate: rounded, well-graded aggregate flows more easily than angular or poorly graded material.
  • Temperature and time: hot weather and waiting time both reduce slump, because the concrete stiffens as it hydrates and loses water.
  • Cement content and fineness: richer, finer mixes need more water for the same slump.

Common mistakes

  • Testing on an uneven, soft or absorbent surface, which changes the shape of the slump.
  • Lifting the cone too fast, or with a twist, which causes false shear slumps.
  • Not rodding evenly, or skipping the layer-below penetration, so the cone is not compacted the same way each time.
  • Adding water on site to fix a low slump. Use an admixture, as approved, instead; extra water lowers strength and causes problems such as the ones described in why concrete cracks on site.
  • Testing a sample taken from the first or last part of the discharge, rather than from the middle of the batch.

Limits of the test

The slump test suits plastic, workable concrete. It is not reliable for very stiff mixes (almost no slump) or for very wet, self-compacting concrete, where a slump-flow test is used instead. It is also only a check on consistency. Quality control still needs cube tests, and good site practice, as covered in why concrete fails on site.

Frequently asked questions

What is a good slump value for concrete?

It depends on the work. Around 50 to 100 mm suits many slabs and beams, while heavily reinforced sections and pumped concrete usually need more. Use the value in the approved mix design.

Does a higher slump mean stronger concrete?

No. For the same mix, a higher slump from added water means lower strength. Slump measures workability, not strength.

How many times should the slump test be done?

As per the specification, commonly for each truck or batch, and whenever the concrete looks different from the approved mix.

What if the slump is too low?

Do not add water. Ask the supplier or engineer about a plasticiser, or reject the batch if it is outside the allowed range.

What is the difference between slump and flow?

Slump measures how much a stiff-to-plastic cone of concrete settles. Flow tests measure how far very wet concrete spreads, and are used when slump would simply collapse.

Related reading: Concrete cube test · Water-cement ratio · How much concrete do I need · Proctor compaction test.

Stop calculating by hand — go Pro

Unlock an ad-free experience plus a growing library of ready-to-use civil-engineering calculators, IS-code cheat-sheets and formula PDFs. From just ₹99.

Go Pro →
Fuel Free Learning Support TheCivilStudies

Keep civil engineering knowledge free — articles, calculators, and practical site guides for everyone.

Choose an amount

100% Secure · Powered by Cashfree

TheCivilStudies Team
TheCivilStudies Team

TheCivilStudies is an independent civil-engineering learning site from India. Our guides explain IS-code provisions, formulas, worked examples and site practice for students and working site engineers. Calculations are checked against the relevant Indian Standard, and articles are updated when codes or practice change. Spotted an error? Tell us in the comments and we will fix it.

Articles: 467